What Is the Melting Point of EVA Granules?

EVA granules are widely used in footwear manufacturing, foam production, and polymer compounding. One common question from material buyers and production engineers is: what is the melting point of EVA granules?

There is no single melting temperature that applies to every EVA grade. EVA is a thermoplastic copolymer, and its melting behavior varies with vinyl acetate (VA) content, molecular structure, crystallinity, and grade formulation. Commercial products may also report a melting range or a differential scanning calorimetry (DSC) peak rather than one universal value.

For example, Dow reports DSC melting points of 98°C for ELVAX 750 and 63°C for ELVAX 150. Both are EVA resin grades, but their VA contents differ. These values demonstrate why manufacturers should check the technical data sheet for the specific material they use.

It is also important to distinguish the melting point of unfoamed EVA resin granules from the processing temperature used in extrusion, injection molding, or foam production. These temperatures describe different things and should not be used interchangeably.

What Is the Melting Point of EVA Granules?

EVA stands for ethylene-vinyl acetate copolymer. It is a thermoplastic polymer made by combining ethylene and vinyl acetate units in a polymer chain.

When EVA resin granules are heated, their crystalline regions gradually lose their ordered structure. The material transitions from a solid polymer into a softened and eventually molten state. Unlike a pure substance with a single sharp melting point, EVA grades may show a melting interval and a characteristic DSC melting peak.

The reported melting temperature depends on the particular grade and the test method used. A supplier may list a DSC melting point, melting temperature, or another thermal property in its technical data sheet. These values should be interpreted according to the manufacturer’s test conditions and terminology.

EVA Resin Granules, Compound Granules, and Other EVA Materials

Not every product described as an EVA granule has the same composition.

  • EVA resin granules: Pellets of the base ethylene-vinyl acetate copolymer supplied as raw material.
  • EVA compound granules: Formulated pellets containing EVA resin and ingredients such as fillers, pigments, processing aids, or other additives.
  • EVA foam: A cellular material produced by foaming an EVA-based compound.
  • EVA hot-melt adhesive: An adhesive formulation that may contain EVA copolymer along with tackifiers, waxes, and other ingredients.

The melting behavior of a formulated compound or adhesive may differ from that of the base EVA resin. Likewise, finished EVA foam does not behave like ordinary unfoamed thermoplastic pellets when reheated.

For manufacturers working with raw materials before foaming, the EVA material manufacturing process provides additional background on material preparation.

Does EVA Have a Fixed Melting Point?

No. EVA does not have one fixed melting point that applies to all commercial grades.

The polymer’s thermal behavior is influenced by its composition and molecular structure. One of the most important factors is the proportion of vinyl acetate in the copolymer.

Vinyl Acetate Content

EVA contains ethylene units and vinyl acetate units. As VA content increases, the regular arrangement of ethylene sequences is disrupted. This generally reduces crystallinity and lowers the melting temperature.

In broad terms, an EVA grade with a higher VA content tends to have a lower melting temperature than a comparable grade with a lower VA content. It may also show greater flexibility and different flow characteristics.

However, VA content is not the only factor. Molecular characteristics, grade design, additives, and measurement conditions can also influence the reported thermal behavior.

Molecular Structure and Crystallinity

Crystalline regions form when sections of polymer chains arrange themselves into ordered structures. These regions contribute to the thermal transitions observed when EVA is heated.

The amount and characteristics of crystalline regions influence the melting behavior. Differences in polymer chain structure and molecular characteristics can therefore produce different thermal results, even among grades with similar VA content.

Melt Flow Rate

Melt flow rate (MFR), sometimes called melt index, describes how much molten polymer flows through a standardized test apparatus under specified conditions.

It is an indicator of melt flow behavior, not a measurement of melting point. Two EVA grades may have similar VA content but different MFR values, which can affect how they flow during processing.

A higher MFR does not automatically mean a lower melting temperature. Manufacturers should evaluate MFR and thermal properties as separate characteristics when comparing materials.

Additives and Formulation

EVA compound granules may contain fillers, pigments, processing aids, crosslinking ingredients, or other additives. These ingredients can influence processing behavior and the thermal response of the formulated material.

For this reason, the DSC melting point of a base EVA resin should not automatically be applied to a compound made from that resin. Buyers should request technical data for the actual grade or formulation being used.

EVA Melting Point Examples by Commercial Grade

Manufacturer data sheets show how much melting behavior can vary among commercial EVA grades.

The following examples are taken from Dow’s ELVAX EVA copolymer resin grade selection guide. The reported values are DSC melting points, not recommended processing temperatures.

Manufacturer and GradeVA ContentReported DSC Melting Point
Dow ELVAX 7509%98°C
Dow ELVAX 46018%88°C
Dow ELVAX 36025%78°C
Dow ELVAX 26528%73°C
Dow ELVAX 15032%63°C

These examples show a general trend: the listed grades with higher VA content have lower reported DSC melting points. They are specific commercial products, not a universal EVA melting-point chart.

A second example comes from Borealis. Its OE5918 EVA copolymer data sheet reports:

PropertyReported Value
GradeOE5918
VA Content18%
Melting Temperature82°C
Test MethodISO 11357-3

The Borealis value is reported for one specific industrial grade. It should not be assumed to apply to every EVA grade with 18% VA. Differences in polymer characteristics and product specifications can produce different results.

For grade comparisons, consult the Dow ELVAX EVA resin grade selection guide and the Borealis OE5918 EVA copolymer technical data sheet. The values are manufacturer-reported typical properties, not guaranteed specifications for every production batch.

EVA Melting Point vs. Processing Temperature

The melting point of EVA and its processing temperature are related, but they are not the same measurement.

Understanding the difference is important because a resin’s DSC melting peak cannot be used directly as the temperature setting for every production machine.

DSC melting peak temperature is the temperature at the peak of a melting-related event on a differential scanning calorimetry curve. It is measured under controlled laboratory conditions.

Melting range describes the interval over which melting occurs. The material may begin melting before reaching its peak temperature and complete the transition at a higher temperature.

Melt temperature refers to the temperature of the polymer after it has melted during processing. It may be measured in the material flow path rather than inferred from a machine’s heating-zone setting.

Processing temperature refers to the temperatures used or measured during a particular operation. These may include barrel zones, die temperatures, mold temperatures, or other equipment settings.

Vicat softening temperature is a separate test result that measures resistance to penetration under specified conditions. It is not the melting point.

Actual processing conditions depend on several factors:

  • EVA grade and VA content
  • Melt flow rate and melt viscosity
  • Processing method, such as extrusion or injection molding
  • Equipment design and screw configuration
  • Shear heating and material residence time
  • Compound formulation and required product quality

For example, extrusion requires consideration of material flow, screw design, pressure, and residence time. Injection molding has different equipment and mold-filling requirements. EVA foam production may involve additional formulation and crosslinking considerations.

The Celanese EVA general extrusion guide explains how VA content and melt index influence extrusion behavior. It also emphasizes that processing recommendations are guidelines for the relevant extrusion applications, not universal settings for injection molding or foaming.

Excessive heat exposure or unsuitable residence times can cause polymer degradation. Manufacturers should follow the supplier’s grade-specific recommendations rather than applying one processing temperature to every EVA material.

How Is EVA Melting Temperature Measured?

Differential scanning calorimetry (DSC) is a common method for evaluating the melting behavior of polymers, including EVA.

During a DSC test, a small material sample is subjected to a controlled heating program. The instrument monitors the heat flow associated with thermal transitions as the sample is heated.

When the polymer’s crystalline regions melt, the DSC curve shows a corresponding thermal event. The result can be used to identify several points:

  • Onset temperature: The point where the melting-related event begins.
  • Peak temperature: The temperature at the maximum of the melting peak.
  • Endset temperature: The point where the melting event is considered complete.

These values describe different parts of the thermal transition. A manufacturer’s reported melting temperature should therefore be read in the context of its test method and reporting convention.

ISO 11357-3:2025 specifies a method for determining melting and crystallization temperatures and enthalpies of crystalline or partially crystalline plastics using conventional DSC. The 2025 edition is the current published edition, replacing ISO 11357-3:2018.

When comparing EVA grades, manufacturers should check whether the reported value is an onset, peak, or another characteristic temperature. Test conditions and reporting conventions can affect the result, so values from different sources should not automatically be treated as perfectly equivalent.

EVA Granules vs. EVA Foam: Do They Have the Same Melting Behavior?

No. Unfoamed EVA granules and finished EVA foam have different structures and may behave differently when heated.

Unfoamed EVA resin granules are thermoplastic pellets. When heated sufficiently, they soften and melt, allowing the material to flow during suitable processing operations.

Finished EVA foam contains a cellular structure formed during manufacturing. Depending on the formulation and production method, it may also contain crosslinking agents, foaming agents, fillers, and other additives.

Crosslinked EVA foam does not behave like ordinary thermoplastic resin pellets when reheated. Its polymer network restricts the ability of the material to flow like an unfoamed thermoplastic melt. Heating may instead cause softening, deformation, shrinkage, or thermal degradation, depending on the material and exposure conditions.

For this reason, the melting point of an EVA resin grade should not be used as the melting point of a finished EVA foam product. The thermal behavior of foam depends on its formulation, cellular structure, and degree of crosslinking.

The EVA foam manufacturing process explains how the production route changes the material from an EVA-based compound into a cellular product.

Why EVA Melting Behavior Matters in Footwear Manufacturing

EVA melting behavior influences raw material selection and downstream processing. A grade that works well in one production method may not be suitable for another without adjustments to the formulation or process.

During material preparation and compounding, manufacturers need to consider the compatibility of the base resin with fillers, additives, and other ingredients. The EVA compounding process provides further information on how these materials are prepared for production.

For injection molding, melt flow and viscosity affect how the material fills the mold and forms the intended component. Selecting a suitable grade requires more than checking its melting point. The material’s MFR, formulation, and processing characteristics must also be considered. Manufacturers can learn more about the equipment in this guide to the EVA injection molding machine.

For foamed footwear components, the base material is processed as part of a formulated system. Foaming behavior, crosslinking, mold design, and process control all influence the final product. The appropriate EVA foaming machine is selected according to the intended production process and product requirements.

ONE-NINE Machinery Co., Ltd. has more than 40 years of experience in footwear machinery manufacturing. Under the KING SUN brand, the company provides EVA footwear processing equipment and production-line solutions. Its machinery supports downstream manufacturing operations; the correct material melting and processing conditions still need to be established using the supplier’s technical data and production trials.

Conclusion

The EVA granules melting point depends on the specific resin grade, particularly its VA content, molecular characteristics, and crystalline structure. Commercial EVA grades can have noticeably different DSC melting temperatures, so one value should not be applied to every EVA material.

Manufacturers should also distinguish the DSC melting peak from the actual melt temperature, processing temperature, and Vicat softening temperature. These measurements describe different material behaviors and serve different purposes.

When selecting EVA granules for footwear production, review the supplier’s technical data sheet, including VA content, MFR, and thermal properties. Then confirm processing conditions through grade-specific recommendations and production trials. This approach helps manufacturers match the material to their compounding, injection molding, or foaming process and maintain consistent finished-product quality.

Similar Posts

Leave a Reply

Your email address will not be published. Required fields are marked *